AMSOIL Synthetic
SG Series EP Gear Oils |
| |
SGK
ISO 100 |
SGL
ISO 150 |
SGM
ISO 220 |
SGN
ISO 320 |
SGO
ISO 460 |
SGP
ISO 680 |
| 2 EP |
3 EP |
4 EP |
5
EP |
6
EP |
7 EP |
8 EP |
| AGMA Synthetic Gear |
3S |
4S |
5S |
6S |
7S |
8S |
| ISO VG —
ASTM D-2422 |
100 |
150 |
220 |
320 |
460 |
680 |
| VK 100°C —
ASTM D-445 |
13.52 |
17.82 |
22.49 |
28.80 |
36.11 |
48.21 |
| VK 40°C —
ASTM D-445 |
100.79 |
149.78 |
220.26 |
312.67 |
433.14 |
659.85 |
| Viscosity Index —
ASTM
D-2270 |
134 |
132 |
125 |
125 |
125 |
125 |
| SPGR —
ASTM D-1298 |
0.8591 |
0.8654 |
0.8745 |
0.8772 |
0.8811 |
0.8866 |
| Density —
ASTM D-1298 |
7.155 |
7.207 |
7.283 |
7.305 |
7.338 |
7.384 |
| Flash Point °C
(°F) —
ASTM D-92 |
246
(475) |
248
(478) |
252
(486) |
246
(475) |
246
(475) |
244
(471) |
| Fire Point °C
(°F) —
ASTM D-92 |
276
(529) |
282
(540) |
286
(547) |
286
(547) |
286
(547) |
286
(547) |
| Pour Point °C
(°F) —
ASTM D-97 |
-45
(-49) |
-42
(-44) |
-40
(-40) |
-235
(-31) |
-35
(-31) |
-33
(-27) |
| Noack —
DIN 51581 |
5.41% |
5.59% |
5.05% |
5.15% |
5.63% |
5.25% |
Four-Ball Wear Test —
(40 kg, 1200 rpm, 75°C,
60 min.) ASTM D-4172 Mod. |
0.41 |
0.35 |
0.35 |
0.35 |
0.33 |
0.31 |
Copper Strip Corrosion
Test —
ASTM D-130
121°C (250°F), 3 hrs. |
1B |
1B |
1B |
1B |
1B |
1B |
| Timken OK Load, EP —
ASTM D-2782 |
75 lbs. |
75 lbs. |
75 lbs. |
75 lbs. |
75 lbs. |
75 lbs. |
Four-Ball
EP ASTM D-2783 —
Weld Point, Kg
Load Wear Index, Kgf |
315
60 |
315
60 |
315
60 |
315
60 |
315
60 |
315
60 |
| FZG, Passed Stage ASTM
D5182 |
12 |
12 |
12 |
12 |
12 |
12 |
| Channel Point @ -40°C
(-40°F) —
FTM 3456.2 |
Non